ATTACH_Tech_Data.pdf

PDF 82 KB Posted

Attached to
SPE1C1-23-R-0017 Radio Contaminant Protective (RCP) Coveralls - Solicitation
Solicitation number
SPE1C1-23-R-0017
Issued by

View the file

Other files

File Type Posted
SF30_SPE1C123R00170002.pdf PDF
SPE1C123R0017-Amend 0001.pdf PDF
SF33_SPE1C123R0017.PDF PDF

On GovTribe

Work with this file

  • Download the original file
  • Contacts named in this file
  • Similar government files
  • Ask GovTribe AI about this file

Text version

PGC03737-UPDATE 08/16/2022

RCP COVERALLS

RA001: THIS DOCUMENT INCORPORATES TECHNICAL AND/OR QUALITY REQUIREMENTS (IDENTIFIED BY AN 'R' OR AN 'I' NUMBER) SET FORTH IN FULL TEXT IN THE DLA MASTER LIST OF TECHNICAL

AND QUALITY REQUIREMENTS FOUND ON THE WEB AT:

http://www.dla.mil/HQ/Acquisition/Offers/eProcurement.aspx

FOR SIMPLIFIED ACQUISITIONS, THE REVISION OF THE MASTER IN EFFECT ON THE SOLICITATION ISSUE DATE OR THE AWARD DATE CONTROLS. FOR LARGE ACQUISITIONS, THE REVISION OF THE

MASTER IN EFFECT ON THE RFP ISSUE DATE APPLIES UNLESS A SOLICITATION AMENDMENT

INCORPORATES A FOLLOW-ON REVISION, IN WHICH CASE THE AMENDMENT DATE CONTROLS.

RQ009: INSPECTION AND ACCEPTANCE AT ORIGIN

RP001: DLA PACKAGING REQUIREMENTS FOR PROCUREMENT

COVERALLS SHALL BE MADE IN ACCORDANCE WITH NCTRF PD 02-11 version "A" DATED 31 MARCH 2021 PATTERN DATE: 20 OCTOBER 2010 STANDARD SAMPLE OF CLOTH, TWILL, POLYESTER AND

COTTON, YELLOW 3511 IS AVAILABLE AND IS APPLICABLE FOR SHADE ONLY. ROLL #10342

INTERIM SPECIFICATION CHANGE FOR NCTRF PD 02-11 version "A":

PAGE 20, TABLE IX, UNDER EXAMINE COLUMN, ELASTIC WEBBING (BACK)SECTION, DELETE "222"

UNDER CLASSIFICATION/MINOR COLUMN.

ADDITIONAL INFORMATION FOR JJ-W-155:

INTERIM STANDARD SAMPLE FOR FOLIAGE GREEN 504 IS MIL-C-44436, ROLL #3729 (THE FOLIAGE

GREEN 502 AREA OF THE PATTERN),AND REFERENCED FOR SHADE ONLY. THIS STANDARD IS

TEMPORARY UNTIL FURTHER NOTICE. THIS APPLIES TO TYPE I, CLASS 6 AND TYPE I, CLASS 11.

INTERIM SPECIFICATION CHANGES TO JJ-W-155H:

PAGE 8, TABLE I, ACROSS FROM CLASS 3, UNDER MIN. YARNS PER INCH: DELETE "100" AND

SUBSTITUTE "100 12/".

PAGE 10, TABLE I, ACROSS FROM CLASS 29, UNDER MIN. YARNS PER INCH: DELETE FOOTNOTE

"6/" AND SUBSTITUTE FOOTNOTE "10/".

UNDER FOOTNOTE 11/: ADD "12/ 100 YARNS PER INCH OF 24/2 YARN OR 136 YARNS PER INCH OF

40/2 WITH 2 YARNS PER SHED."

PAGE 12, PARA. 3.10.1 DELETE IN ITS ENTIRETY AND SUBSTITUTE "3.10.1 AQUEOUS COPPER-8- QUINOLINOLATE. THE WEBBING SPECIFIED IN 3.10 SHALL BE MILDEW TREATED WITH AQUEOUS COPPER 8-QUINOLINOLATE OR OTHER APPROVED AQUEOUS BASED MILDEW INHIBITOR. BECAUSE OF THE TIME NECESSARY TO CONDUCT FULL EVALUATION, ONLY THOSE TREATMENTS ALREADY APPROVED AND SO LISTED IN THE INVITATION FOR BIDS OR REQUESTS FOR PROPOSAL SHALL BE CONSIDERED

ACCEPTABLE FOR THE RELATED PROCUREMENT."

PAGE 26, PARA 4.3.1, LINE 8, BETWEEN "...(SEE 6.4)." AND "THE STARTING GAGE..." INSERT "AS AN ALTERNATE, ASTM-D4964 MAY BE USED TO DETERMINE ELASTIC LOOP TENSION AT SAME REQUIRED PERCENT ELONGATION AND UNDER SAME CARRIAGE LOAD PARAMETERS AS SPECIFIED IN

TABLE III (I.E. FOR TYPE 1, CI 20 ELASTIC SET CRE CYCLE TO MAXIMUM 30 LBS. AND

DETERMINE LOOP TENSION ON THIRD CYCLIC UPLOAD CURVE AT 50% ELONGATION). IF ALTERNATE TM IS USED, THEN ALLOW A +10% FACTOR TO MAXIMUM TENSION REQUIREMENT IN TABLE III."

APPROVED AQUEOUS MILDEW TREATMENTS FOR:

MIL-W-43638 WEBBING, TEXTILE, WOVEN FOR TENT FRAMING;

MIL-W-5665, WEBBING, TEXTILE, COTTON WARP;

MIL-W-530, WEBBING, TEXTILE, COTTON GENERAL PURPOSE, NATURAL OR IN COLORS;

MIL-T-43566, TAPE, TEXTILE, COTTON OR POLYESTER, GENERAL PURPOSE, NATURAL OR IN

COLORS,

JJ-W-155, WEBBING, TEXTILE, (COTTON,ELASTIC):

PRODUCT SUPPLIER

CUNILATE 2002 MORTON INTERNATIONAL, INC

150 ANDOVER STREET

DANVERS, MA. 01923

TEL: (508-774-3100)

ACCEPTABLE ALTERNATE MILDEW TREATMENT FOR 2,2'

METHYLENE-BIS-(4-CHLOROPHENOL)

1. WHEN A SPECIFICATION SPECIFIES "2,2'

METHYLENE-BIS-(4- CHLOROPHENOL)" MILDEW RESISTANT

TREATMENT FOR COTTON TEXTILE MATERIALS, "RO-59"

IS APPROVED AS AN ALTERNATIVE TREATMENT AND IS

AUTHORIZED FOR USE. THIS CHANGE APPLIES TO

PENDING AND FUTURE CONTRACTS USING TEXTILE

MATERIALS THAT SPECIFY THE SUBJECT MILDEW

RESISTANT TREATMENT.

2. THE PRODUCT MAY BE OBTAINED FROM:

RO-59 INC.

1 CABOT PL #3

STOUGHTON, MA 02072

TELEPHONE (781) 264-1213

POC: MR. RONNIE BENDER

3. THE TEXTILE MATERIALS TREATED WITH RO-59

MILDEW INHIBITOR TREATMENT SHALL BE TESTED IN

ACCORDANCE WITH AATCC TEST METHOD

30 - ANTIFUNGAL ACTIVITY, ASSESSMENT ON TEXTILE

MATERIALS: MILDEW AND ROT RESISTANCE OF TEXTILE

MATERIALS, TEST III. THE TREATED MATERIAL SHALL

NOT EXHIBIT "MACROSCOPIC GROWTH

(VISIBLE TO THE EYE)".

"MIL-DTL-32075: LABEL FOR CLOTHING, EQUIPAGE,

AND TENTAGE, GENERAL USE REPLACES DDD-L-20

INTERIM SPECIFICATION CHANGES TO MIL-DTL-32075:

PAGE 6, TABLE I, "PHYSICAL REQUIREMENTS OF THE

TYPE VI FINISHED LABEL." UNDER "TEARING

STRENGTH" DELETE: "(LB.) MINIMUM" AND

SUBSTITUTE: "(GNS) MINIMUM."

PAGE 12, PARA 3.3.2.17, AFTER "NSN" ADD

"AND THE UNIVERSAL PRODUCT CODE (UPC)

SUPPLIED BY THE GOVERNMENT, FOR ALL NSNs."

ADDITIONAL INFORMATION: FED-STD-751 HAS BEEN

CANCELLED AND REPLACED BY ASTM-D-6193, 4/98

STANDARD PRACTICES FOR STITCHES AND SEAMS.

THIS STANDARD SHOULD BE USED IN PREFERENCE

TO FED-STD-751.

ADDITIONAL INFORMATION FOR MIL-I-45208:

NOTE: MIL-I-45208 HAS BEEN CANCELLED AND REPLACED BY THE FOLLOWING: INTERNATIONAL

STANDARDS ISO 9001:2008

OR AMERICAN SOCIETY FOR QUALITY ASQ 2008 VERSION.

ADDITIONAL INFORMATION FOR MIL-STD-105E:

MIL-STD-105E, dated 10 May 1989, is hereby canceled.

Users are cautioned to evaluate these documents for their particular application before citing it as a replacement document.

(Copies of ANSI/ASQ Z1.4 are available online at www.asq.org or ASQ Distribution Center, 5131 S. Third Street, Milwaukee, Wisconsin 53207-6028.)

INCLUDE T0795 OBJECT TEXT ID ST

MIL-STD-129R w/CHANGE 2 - DEPARTMENT OF DEFENSE STANDARD PRACTICE MILITARY MARKING FOR

SHIPMENT AND STORAGE

DATED: 27 SEPTEMBER 2019

INTERIM CHANGES:

OMISSION OF MARKINGS ON EXTERIOR SHIPPING CONTAINERS OF ITEMS

IN THE DLA TROOP SUPPORT CLOTHING AND TEXTILE (C&T) DIRECTORATE:

THE NOMENCLATURE AND MANUFACTURER'S NAME (WHEN THE NAME IDENTIFIES THE MATERIAL) SHALL

BE OMITTED FROM ALL EXTERIOR SHIPPING CONTAINERS OF DLA TROOP SUPPORT C&T ITEMS,

REGARDLESS OF MODE OF SHIPMENT.

IF THE MANUFACTURER'S NAME DOES NOT IDENTIFY THE MATERIAL AS BEING CLOTHING, IT MAY REMAIN. NSNS SHALL BE SHOWN ON ALL SHIPPING CONTAINERS OF C&T ITEMS, THE PACKING LIST SHALL BE PLACED INSIDE THE LAST CONTAINER TO BE LOADED FOR EACH SHIPMENT. THE WORDS

"PACKING LIST HERE" SHALL BE STENCILED, NOT HAND LETTERED, ON THE CONTAINER.

MIL-STD-147E w/CHANGE 2

27 JUNE 2019

DEPARTMENT OF DEFENSE

STANDARD PRACTICE

PALLETIZED UNIT LOADS

ADDITIONAL INFORMATION FOR FED-STD-191:

INTERIM CHANGES TO FED-STD-191A:

1200 AATCC-20 FIBER ANALYSIS: QUALI-

. TATIVE - OR

. ASTM-D-276 IDENTIFICATION OF FI-

. BERS IN TEXTILES.

2011 N/A

2020 PRESENCE OF LABILE SULFUR: IN TEX-

. TILE MATERIALS WITH LEAD ACETATE,

. TWO 1.50 +/- 0.01 GRAM SAMPLES FROM

. EACH MATERIAL SHALL BE TESTED. EACH

. OF THE TWO SAMPLES SHALL BE CUT

. INTO VERY SMALL PIECES AND PLACED

. INTO SEPARATE TEST TUBES. THE SAM-

. PLES SHALL BE SUBMERSED IN A STAN-

. NOUS CHLORIDE SOLUTION THAT CONTAIN

. 100 GRAMS OF STANNOUS CHLORIDE

. CRYSTALS ACS IN 100 MILLILITERS OF

. HYDROCHLORIC ACID ACS (35% CONCEN-

. TRATION) AND 50 MILLILITERS OF

. DISTILLED WATER. A FILTER PAPER

. WET OUT WITH A 5.0% LEAD ACETATE

. SOLUTION SHALL BE PLACED OVER TOP

. OF THE TEST TUBE. THE LEAD ACE-

. TATE SOLUTION SHALL BE PLACED OVER

. TOP OF THE TEST TUBE. THE LEAD

. ACETATE SOLUTION CONTAINS 5.0 GRAMS

. OF LEAD ACETATE CP REAGENT GRADE &

. ENOUGH DISTILLED WATER TO MAKE UP A

. 100 MILLILITER SOLUTION; IF THE

. SOLUTION IS NOT CLEAR, ADD A FEW

. DROPS (ONE AT A TIME) OF GLACIAL

. ACETIC ACID UNTIL THE SOLUTION IS

. CLEAR. THE TEST TUBE CONTAINING

. THE TEXTILE SAMPLE, STANOUS CHLOR-

. OF THE TEST TUBE. THE LEAD ACE-

. TATE SOLUTION SHALL BE PLACED OVER

. TOP OF THE TEST TUBE. THE LEAD

. ACETATE SOLUTION CONTAINS 5.0 GRAMS

. OF LEAD ACETATE CP REAGENT GRADE &

. ENOUGH DISTILLED WATER TO MAKE UP A

. 100 MILLILITER SOLUTION; IF THE

. SOLUTION IS NOT CLEAR, ADD A FEW

. DROPS (ONE AT A TIME) OF GLACIAL

. ACETIC ACID UNTIL THE SOLUTION IS

. CLEAR. THE TEST TUBE CONTAINING

. THE TEXTILE SAMPLE, STANOUS CHLOR-

. IDE AND WET FILTER PAPER SHALL BE

. HEATED OVER AL LOW FLAME UNTIL THE

. SOLUTION IS BOILING. THE SOLUTION

. SHOULD NOT BE HEATED FOR MORE THAN

. 15 SECONDS. A BROWN TO BLACK STAIN

. ON THE FILTER PAPER SHOULD BE EVAL-

. UATED AS FOLLOWS:

. FREE - THE FILTER PAPER SHOWS

. NO DISCOLORATION OR

. STAINING OF ANY KIND.

. SLIGHT - THE FILTER PAPER SHOWS A

. LIGHT TAN OR LIGHT BROWN

. DISCOLORATION STAIN.

. MODERATE - THE FILTER PAPER SHOWS A

. DARK BROWN DISCOLORATION

. STAIN.

. SEVERE - THE FILTER PAPER SHOWS A

. BLACK COLOR STAIN.

2100 AATCC-20A FIBER ANALYSIS: QUALI-

. TATIVE - OR -

. ASTM-D-629 QUANTITATIVE ANALYSIS OF

. TEXTILES.

2610 AATCC-20A FIBER ANALYSIS: QUALI-

. TATIVE - OR -

. ASTM-D-629 QUANTITATIVE ANALYSIS OF

. TEXTILES

2811 AATCC-81 PH OF WATER-EXTRACT FROM

. BLEACHED TEXTILES - OR -

. ASTM-D-2165 PH OF AQUEOUS EXTRACTS

. OF WOOL & SIMILAR ANIMAL

. FIBERS.

4010 ASTM-D-1907 LINEAR DENSITY OF YARN

. (YARN NUMBER) BY THE

. SKEIN METHOD.

4050 ASTM-D-1423 TWIST IN YARNS BY THE

. DIRECT-COUNTING METHOD.

4100 ASTM-D-2256 TENSILE PROPERTIES OF

. YARN BY THE SINGLE-

. STRAND METHOD

. (TESTING SPEED SHALL BE

. 12 +/- 0.5 IN/MIN & A 10

. INCH GAUGE LENGTH SHALL

. BE USED).

5030 ASTM-D-1777 THICKNESS OF TEXTILE

. METHODS

. NOTE: A THICKNESS GAUGE

. OF THE DEAD-WEIGHT TYPE EQUIPPED

. WITH A DIAL GRADUATED TO READ DI-

. RECTLY TO 0.0001 INCHES SHALL BE

. USED. THE PRESSER FOOT SHALL BE

. CIRCULAR, WITH A DIAMETER OF 0.375

. +/- 0.0001 INCHES AND WITH THE MOV-

. ING PARTS WEIGHTED TO APPLY A TOTAL

. LOAD OF 3.4 +/- 0.1 POUNDS PER

. SQUARE INCH TO THE SPECIMEN. THE

. ANVIL SHALL BE NOT LESS THAN 0.250

. INCHES IN DIAMETER. THE PRESSER

. FOOT AND ANVIL SURFACE SHALL BE NOT

. LESS THAN 0.250 INCHES IN DIAMETER.

. THE PRESSER FOOT AND ANVIL SURFACE

. SHALL BE PLANED TO WITHIN 0.0001

. INCHES AND SHALL BE PARALLEL TO EACH

. OTHER TO WITHIN 0.0001 INCHES. THE

. MICROMETER SHALL BE CAPABLE OF RE-

. PEATING ITS READING TO 0.0005 INCHES

. AT ZERO SETTING OR ON A STEEL GAUGE

. BLOCK. THE FIVE SPECIMENS SHALL BE

. TESTED AND THE RESULTS AVERAGED AND

. REPORTED TO THE NEAREST 0.001 INCH.

5041 ASTM-D-3776 MASS PER UNIT AREA

. (WEIGHT) OF FABRIC -

. OPTION A

5050 ASTM-D-3775 FABRIC COUNT OF WOVEN

. FABRIC.

5100 ASTM-D-5034 BREAKING FORCE & ELON-

. GATION OF TEXTILE FABRIC

. (GRAB TEST), G-E OR G-T.

5500 AATCC-70 WATER REPELLENCY: TUMBLE

. JAR DYNAMIC ABSORPTION

5556 AATCC-96 DIMENSIONAL CHANGES IN

. COMMERCIAL LAUNDERING OF

. WOVEN & KNITTED FABRICS

. EXCEPT WOOL (TEST VI,A).

5610 AATCC-61 COLORFASTNESS TO LAUND-

. ERING, HOME & COMMERCIAL

. ACCELERATED (TEST 3A).

5622 N/A

5660 AATCC-16 COLORFASTNESS TO LIGHT

. (OPTION A).

5671 AATCC-111A WEATHER RESISTANCE: SUN

. ARC LAMP EXPOSURE WITH

. WETTING

5680 AATCC-15 COLORFASTNESS TO

. PERSPIRATION.

ADDITIONAL INFORMATION FOR FED-STD-191:

FED-STD-191A NOTICE 7, DATED AUGUST 9, 2000 IS HEREBY INACTIVE FOR NEW DESIGN. WHEN NOT USING FED-STD-191, SEE INTERIM CHANGES TO END ITEM SPECIFICATION FOR REPLACEMENT

ASTM.

INTERIM CHANGES TO FED-STD-191A:

TEST METHOD 5202, PARA. 5.3, DELETE FIRST SENTENCE AND SUBSTITUTE: "THE SPECIMEN

SHALL BE CLAMPED FIRMLY, WITH ONE END FLUSH WITH THE OUTER EDGE OF THE VISE, SUCH THAT ONE INCH OF SPECIMEN LIES WITHIN THE CLAMP AND ONE INCH OF THE SPECIMEN EXTENDS BEYOND THE CENTER OF ROTATION (FACE OF THE VISE), AND WITH THE LONG EDGE PARALLEL TO THE FACE

OF THE DIAL PLATE".

TEST METHOD 5309.1 ABRASION RESISTANT OF TEXTILE WEBBING. PAGE 1, PARA 4.1.2,LINE 4:

DELETE "B-97" AND SUBSTITUTE "B-91".

THE FOLLOWING METHODS ARE IDENTIFIED AS SPECIFYING OZONE DEPLETING SUBSTANCES: 1100, 1200, 1240, 1400, 1410, 1500, 1510,1520,1530, 1540, AND 1550. PARA 5.1 OF THESE TEST

METHODS REQUIRE THE USE OF 1,1,1- TRICHLOROETHANE, ALCOHOL OR ETHER. 1,1,1-

TRICHLORETHANE IS AN OZONE DEPLETING SUBSTANCE (METHYL CHLOROFORM) AND IS THEREFORE PROHIBITED. THE USE OF EITHER ALCOHOL OR ETHER IS REQUIRED WHEN THESE METHODS ARE IN

BASIC OR ANY REFERENCED DOCUMENT.

METHOD 5202, STIFFNESS OF CLOTH, DIRECTIONAL; CANTILEVER BENDING METHOD. PAGE 2,

PARA. 5.3 DELETE FIRST SENTENCE AND SUBSTITUTE WITH THE FOLLOWING: "THE SPECIMEN SHALL BE CLAMPED FIRMLY, WITH 1 END FLUSH WITH THE OUTER EDGE OF THE VISE, SUCH THAT 1" OF THE SPECIMEN LIES WITHIN THE CLAMP AND 1" OF THE SPECIMEN EXTENDS BEYOND THE CENTER OF ROTATION (INNER FACE OF THE VISE) AND WITH THE LONG EDGE PARALLEL TO THE FACE OF THE

DIAL PLATE."

METHOD 5556.1, MOBILE LAUNDRY EVALUATION FOR TEXTILE MATERIALS, PAGE 5, PARA. 5.2.2, LINE 8: DELETE SENTENCE BEGINNING WITH "THE SPECIMENS AND BALLAST" IN ITS ENTIRETY AND SUBSTITUTE WITH THE FOLLOWING: "THE SPECIMENS AND BALLAST SHALL BE SEPARATED, OPENED TO FULL WIDTH AND PLACED IN A PRE-HEATED DRYER HAVING A STACK TEMPERATURE OF 140-180 DEG. F. THIS TEMPERATURE RANGE CORRESPONDS TO A SETTING OF "HIGH" ON THE TEMPERATURE INDICATOR ON THE DRYER. DRYING SHALL CONTINUE FOR 45-60 MINUTES OR UNTILSAMPLES ARE

DRY IN A ROTATING TUMBLE DRYER."

PAGE 5, PARA. 5.2.3, LINE 8: DELETE SENTENCE BEGINNING WITH "THE SPECIMENS AND

BALLAST" IN ITS ENTIRETY AND SUBSTITUTE WITH THEFOLLOWING: "THE SPECIMENS AND BALLAST SHALL BE SEPARATED, OPENED TO FULL WIDTH AND PLACED IN A PRE-HEATED DRYER HAVING A STACKTEMPERATURE OF 140-180 DEG. F. THIS TEMPERATURE RANGE CORRESPONDS TO A SETTING OF "HIGH" ON THE TEMPERATURE INDICATOR ON THE DRYER. DRYING SHALL CONTINUE FOR 35-40

MINUTES OR UNTIL SAMPLES ARE DRY."

METHOD 5931, ELECTROSTATIC DECAY OF FABRICS; DETERMINATION OF PAGE 1, PARA. 3: AFTER NUMBER OF DETERMINATIONS ADD "PER SAMPLE UNIT". PAGE 1, PARA. 4: DELETE "APPARTUS"

AND SUBSTITUTE "APPARATUS". PAGE 1, PARA. 5.1, LINE 3: AFTER "AT"

DELETE"APPROXIMATELY".

PAGE 2, PARA. 5.2, LINES 2, AND 5: AFTER "OF" ADD "+-". LINE 6: AFTER "TO" ADD "+-".

PAGE 2, PARA. 5.3: DELETE IN ITS ENTIRETY AND SUBSTITUTE WITH THE FOLLOWING:"5.3 MOUNT A SPECIMEN TIGHTLY ACROSS THE ELECTRODES, CENTERING IT OVER THE SENSOR OPENING. THE SURFACE OF THE TEST SPECIMEN (BACK OR FRONT) SHALL FACE THE SENSOR. RECORD (OPTIONAL) THE RESIDUAL CHARGE LEVEL ON THE SAMPLE AS SEEN BY THE SENSOR, INCLUDING POLARITY.

NOTE THAT TEST SAMPLES WITH THE RESIDUAL CHARGE LEVELS OF LESS +500 VOLTS YIELD THE BEST RESULTS. APPLY +5000 VOLTS TO THEELECTRODES FOR A PERIOD OF 20 SECS. AT THE END OF THE 20 SECOND PERIOD, THE HIGH VOLTAGE (5000 VOLTS) SHALL BE TURNED OFF ANDTHE SPECIMENS IMMEDIATELY GROUNDED. THE VOLTAGE BEHAVIOR OF THE SPECIMEN WITH RESPECT TO TIME SHALL BE PLOTTED ON THE RECORDER. NOTE: IN SOME CASES, THE TEST EQUIPMENT WILL DISPLAY VOLTAGE AND DECAY TIME INFORMATION AND A CHART RECORDER IS NOT NECESSARY."

PAGE 2, PARA. 5.4, LINE 3: DELETE SENTENCE BEGINNING WITH "IF THE SPECIMEN DID" IN ITS

ENTIRETY.

PAGE 2, PARA. 5.5: DELETE PARAGRAPH IN ITS ENTIRETY AND SUBSTITUTE WITH THE FOLLOWING:

"RECORD THE MAXIMUM VOLTAGE LEVEL(INCLUDING POLARITY) AND DECAY TIME TO 10% OF THE

MAXIMUM VOLTAGE LEVEL ACHIEVED."

PAGE 2, PARA. 5.6, LINE 1: ADD THE FOLLOWING PRIOR TO 1ST SENTENCE: "REVERSE VOLTAGE

POLARITY REPEAT MEASUREMENT, ANDRECORD RESULTS."

PAGE 3, PARA. 6.6: DELETE PARAGRAPH IN ITS ENTIRETY AND SUBSTITUTE WITH THE FOLLOWING:

"THE AVERAGE TIME TO DECAY TO 10%OF THE MAX VOLTAGE SHALL BE INCLUDED FOR EACH OF THE WARP & FILLING DIRECTIONS, AS WELL AS THE OVERALL AVERAGE, FOR EACHFABRIC TESTED.

THESE WILL BE OBTAINED BY AVERAGING THE TEST RESULTS (ABSOLUTE VALUE OF) TOGETHER FOR BOTH VOLTAGEPOLARITIES. UNLESS OTHERWISE STATED IN THE REQUIREMENTS DOCUMENT, THE FABRIC SHALL BE CONSIDERED ACCEPTABLE IF THEAVERAGE MAXIMUM VOLTAGE IN BOTH THE WARP AND FILLING DIRECTIONS IS LESS THAN 4000 VOLTS, AND THE AVERAGE DECAY TIME (TO 10% MAXVOLTAGE) IS GREATER THAN 0.5 SECONDS IN BOTH THE WARP AND FILLING DIRECTIONS. IT

SHALL BE INDICATED WHETHER THE FABRIC ISACCEPTABLE OR NON-ACCEPTABLE."

PAGE 3, PARA. 7.1, SECOND COLUMN, LINE 2: DELETE 406C AND SUBSTITUTE WITH "406D".

AFTER PARA. 7.1, ADD THE FOLLOWING: "7.2 NOTE: IF THE MODEL 406D STATIC DECAY METER, OR EQUIVALENT, IS USED, A CHART RECORDER ISNOT MANDATORY FOR THE TEST."

ALL PACKAGING/PRESERVATION SHALL BE IN ACCORDANCE WITH

ASTM D-3951, STANDARD PRACTICE FOR COMMERCIAL PACKAGING.

INTERIM CHANGES TO A-A-55126B,

THE FOLLOWING CHANGES ARE FOR ALL CURRENT, PENDING AND FUTURE PROCUREMENTS OF THE

SUBJECT DOCUMENT UNTIL SUCH TIME AS THE DOCUMENT IS AMENDED OR REVISED.

PAGE 4. TABLE I, PHYSICAL REQUIREMENTS, CHARACTERISTIC, SHEAR STRENGTH,DELETE LBS/SQ

INCH (MIN), ADD SHEAR STRENGTH, LBS/2 SQ INCH (MIN).

PAGE 5 TABLE II, PHYSICAL REQUIREMENTS; CHARACTERISTIC, LENGTH

DIMENSIONAL STABILITY, % (MAX); LOOP, ALL CLASSES DELETE .0; ADD ALL CLASSES 4.0.

PAGE 7, Paragraph 3.10.2, Change the following title of paragraph from: "Fray resistance of Universal Camouflage Shades" and replace with "Fray resistance of Camouflage Prints"

PAGE 14, Paragraph 7.3.4 Change the following title of paragraph from: Fray resistance for Universal Camouflage Shades." and replace with "Fray resistance for Camouflage Prints."

NSN 015900608, SIZE S-M

NSN 015900609, SIZE L-XL

INSPECTION TEXT:

Twenty (20) coveralls, of one size only, packaged in accordance with ASTM-D-3951, shall be packed in a fiberboard shipping container, style RSC -L, class domestic, grade 275, CF or SF, variety DW with A SW liner.

Each coverall shall be properly folded and then wrapped with a commercial paper strip across the middle with the ends secured by a gummed paper tape.

The shipping containers shall be assembled, closed and reinforced in accordance with ASTM-D-5118 and ASTM-D-1974 as applicable.

ALL MARKINGS, TO INCLUDE BAR CODE, SHALL BE IN ACCORDING WITH THE LASTEST VERSION OF

MIL-STD-129.

Palletization is required in accordance with MIL-STD-147

QUP=020